Outgassing Data Introduction
Material | Data Ref | Mfr. | TML % | CVCM | WVR | Application | Time 1 | Temp 1 | ATM 1 | Time 2 | Temp 2 | ATM 2 | Time 3 | Temp 3 | ATM 3 | Time 4 | Temp 4 | ATM 4 | Year |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
SMRD 4 UNFILLED EPOXY | GSFC09778 | GEV | 1.67 | 0.12 | 0.64 | DAMPER | 16H | 93 | AIR | 48H | 100 | E-4 | 1978 | ||||||
SMRD 4 UNFILLED EPOXY | GSFC09904 | GEV | 1.56 | 0.11 | 0.69 | DAMPER | 16H | 93 | AIR | 96H | 100 | E-4 | 1978 | ||||||
SMRD 432 | GSFC09533 | GEV | 0.94 | 0.15 | 0.17 | POTTING | 48H | 100 | E-2 | 1978 | |||||||||
SMRD 432 (CURRENT) NEW FLEXIBILIZER | GSFC09883 | GEV | 1.19 | 0.14 | 0.21 | POTTING | 16H | 121 | AIR | 1978 | |||||||||
SMRD 432 (CURRENT) NEW FLEXIBILIZER | GSFC09886 | GEV | 1.36 | 0.16 | 0.27 | POTTING | 24H | 71 | AIR | 1978 | |||||||||
SMRD 432 (ORIGINAL) | GSFC09865 | GEV | 1.27 | 0.20 | 0.31 | POTTING | 16H | 121 | AIR | 1978 | |||||||||
SMRD 432 90A WHITE | GSFC09317 | GEV | 1.14 | 0.17 | 0.23 | POTTING | 1978 | ||||||||||||
SMRD 49 EPOXY | GSFC01246 | GEV | 0.98 | 0.05 | POTTING | 1969 | |||||||||||||
SOCKET STRIP BLACK RYNITE PET POLYESTER | GSFC16166 | SAM | 0.56 | 0.23 | 0.11 | SOCKET STRIP | 1987 | ||||||||||||
SOCKET STRIP BLACK RYNITE PET POLYESTER | GSFC16235 | SAM | 0.40 | 0.17 | 0.10 | SOCKET STRIP | 16H | 175 | AIR | 1987 |