SCOTCHCAST 280 A/B AS 2/3 BW EPOXY GSFC27835 MMM 0.51 0.06 0.22 EPOXY 2H 121 AIR 24H 155 AIR 2002
SCOTCHCAST 280 A/B AS 2/3 BW EPOXY GSFC27838 MMM 0.57 0.11 0.18 EPOXY 16H 93 AIR 6H 125 AIR 2002
SCOTCHCAST 280 A/B AS 2/3 BW EPOXY GSFC27868 MMM 0.67 0.22 0.20 EPOXY 2H 121 AIR 24H 155 AIR 2002
SCOTCHCAST 280 A/B AS 2/3 BW EPOXY GSFC27871 MMM 0.78 0.29 0.15 EPOXY 16H 93 AIR 6H 125 AIR 2002
SCOTCHCAST 280 A/B AS 2/3 BW EPOXY GSFC27874 MMM 0.87 0.16 0.21 EPOXY 24H 75 AIR 2002
SCOTCHCAST 280 EPOXY GSFC32221 HYS 0.48 0.05 0.23 POTTING COMPOUND 3H 120 AIR 96H 105 AIR 2010
SCOTCHCAST 280 EPOXY, 1006251000, EXP 6/1/11 - A/B 2/3 GSFC32191 MMM 0.45 0.08 0.21 EPOXY 4H 150 AIR 32H 130 AIR 2010
SCOTCHCAST 280, A/B 2/3 GSFC32437 MMM 0.29 0.00 0.12 POTTING COMPOUND 24H 75 AIR 24H 130 AIR 2011
SCOTCHCAST 280, A/B 2/3 GSFC32440 MMM 0.35 0.01 0.12 POTTING COMPOUND 24H 75 AIR 24H 155 AIR 2011
SCOTCHCAST 281 A/B AS 2/3 BW BLACK EPOXY GSFC18226 MMM 0.73 0.32 0.14 POTTING 16H 93 AIR 6H 125 AIR 1989